Sinf bilan nikel asosidagi qotishmaInconel 601

Amalga oshirish standartlari:ASTM B366 (zarb) ASTM B168 (plastinka/folga) ASTM B166 (tayoq)

 

Kimyoviy tarkibi:

Element

%

Ni

Cr

Al

Mn

Cu

Si

Fe

C

Nb

P

Standart

min

58.0

21.0

1.0

--

--

--

marja

--

--

--

maks

63.0

25.0

1.70

1.0

1.0

0.50

marja

0.10

1.0

0.03

 

Inconel 601

 

Inconel601 Thermocouple Casing 3

 

 

Inconel 601 qotishmasi 1200 darajada mukammal oksidlanish qarshiligiga ega bo'lgan nikel xrom qotishmasi hisoblanadi. Qotishma 601 qattiq siklik termal muhitda oksidlanishni oldini olish uchun zich oksidli qatlam hosil qilishi mumkin. Qotishma mukammal yuqori harorat kuchiga ega va hali ham uzoq vaqt davomida o'zining noyob mustahkamligini saqlab qolishi mumkin. muddatli yuqori haroratli muhitlar.601 qotishmasi oksidlovchi sharoitlarda ham yaxshi korroziyaga chidamliligiga ega.Biroq, 601 qotishmasini yuqori darajada qaytaruvchi va oltingugurtlashtiruvchi muhitda ishlatish tavsiya etilmaydi.

 

 

 

 

Turli xillik Issiqlik bilan ishlov berish Mustahkamlik chegarasi Hosildorlik kuchi Cho'zilish

HBS

Rod qattiq eritma + qarish

650 dan katta yoki unga teng

300 dan katta yoki teng

30% dan katta yoki teng

217

Sovuq haddelenmiş plastinka qattiq eritma + qarish

600 dan katta yoki unga teng

240 dan katta yoki teng

30% dan katta yoki teng

121-177

 

Zichlik Erish nuqtasi

8,12 g/sm2

1320-1370 daraja

 

Ilova

 

 
  • Sinkni payvandlash, tavlash va sinterlash mufel pechlari va Zhen tipidagi pechlar.

  • Radiatsion quvur

  • Telni yumshatish trubkasi

  • Aylanadigan pech va sinterlash pechi

  • Termal (elektr) juft himoya trubkasi

Inconel601 Thermocouple Casing 6

 

yuqori haroratli ishlash

 

Harorat, daraja

Xona harorati 20

100

200

400

550

600

700

Issiqlik kengayish koeffitsienti, in/daraja x 10-6

--

8.5

8.9

9.2

9.5

9.8

10.2

Issiqlik o'tkazuvchanligi, Btu • ft/ft2 • soat • daraja

6.5

11.6

12.7

13.7

14.8

15.8

16.9

Elastik modul, Dinamik psi x 106

29.95

25.43

24.12

22.48

20.54

18.43

16.20

 

 

Harorat, daraja Xona harorati 20

100

200

400

550

Kuchlanish kuchi, ksi

100

90

60

34

18

0.2% Hosildorlik kuchi, ksi

54

48

41

26

15

Uzayish %

45

44

45

70

120

 

 

Harorat, daraja

400

550

600

700

Minimal siljish, 0.0001%/soat ksi

4.1

2.0

0.76

0.43

10000 soatdan keyin buzilish, ksi

6.2

2.6

1.2

0.62

So'rov yuborish